Six Common Casting Defects: Ua thiab Tiv Thaiv Txoj Kev (Part 2)
Hauv qhov txuas ntxiv no, peb npog peb qhov kev cuam tshuam ntau ntxiv thiab lawv cov laj thawj, nrog rau kev tiv thaiv los pab txo qhov tsis xws luag hauv koj qhov kev lag luam foundry.
4. Kov Crack (Kub Crack, Txias Crack)
Nta: Cov kab nrib pleb hauv castings tuaj yeem ncaj lossis tsis sib xws. Cov kab nrib pleb kub feem ntau muaj qhov tsaus grey lossis dub oxidized nto uas tsis muaj xim hlau, thaum cov kab nrib pleb txias muaj qhov zoo nkauj nrog cov xim hlau. Cov kab nrib pleb sab nrauv feem ntau pom ntawm qhov muag liab qab, thaum cov kab nrib pleb sab hauv yuav tsum muaj ntau txoj hauv kev tshawb pom. Cov kab nrib pleb feem ntau tshwm sim ntawm cov ces kaum sab hauv, qhov hloov pauv tuab, lossis qhov chaw uas cov riser txuas nrog cov ntu kub. Cov kab nrib pleb feem ntau cuam tshuam nrog lwm yam tsis xws li porosity thiab slag inclusions.
Ua rau:
- • Hlau pwm casting zoo li tsim cov kab nrib pleb vim cov pwm tsis muaj qhov hloov pauv, ua rau kom txias sai thiab muaj kev ntxhov siab ntau ntxiv hauv qhov casting.
- • Qhib cov pwm ntxov dhau los lossis lig dhau lawm, lossis tsis tsim nyog lub kaum sab xis, tuaj yeem tsim kev ntxhov siab.
- • Cov khaubncaws sab nraud povtseg lossis cov kab nrib pleb hauv cov pwm tuaj yeem ua rau cov kab nrib pleb.
Txoj kev tiv thaiv:
- • Ua kom muaj kev hloov pauv zoo ib yam hauv cov phab ntsa casting kom txo cov kev ntxhov siab.
- • Kho cov txheej tuab kom cov cua txias tsis sib xws, txo kev ntxhov siab.
- • Tswj cov pwm pwm kub, kho pwm rake, thiab tswj cov tub ntxhais tawg lub sij hawm kom pom kev txias.
- • Siv cov pwm tsim kom tsis txhob muaj kab nrib pleb.
5. Txias kaw (Bad Fusion)
Nta: Txias kaw zoo li seams los yog nto kab nrib pleb nrog puag ncig, qhia tias tsis muaj kev sib xyaw kom zoo. Lawv feem ntau tshwm sim nyob rau sab saum toj phab ntsa ntawm casting, nyob rau hauv nyias kab rov tav los yog ntsug nto, nyob rau hauv lub hlws ris ntawm tuab thiab nyias phab ntsa, los yog nyias panels. Kev kaw qhov txias txias tuaj yeem ua rau tsis tiav casting, ua rau cov txheej txheem tsis muaj zog.
Ua rau:
- • Kev tsim cov pa tsis zoo hauv cov pwm hlau.
- • Ua haujlwm kub qis dhau.
- • Cov txheej txheej tsis zoo lossis tsis zoo, txawm tias yog vim tib neeg yuam kev lossis cov khoom siv tsis zoo.
- • Cov neeg khiav dej num tsis raug.
- • Nqus pouring ceev.
Txoj kev tiv thaiv:
- • Tsim kom muaj qhov khiav thiab tso pa kom zoo kom muaj cua txaus.
- • Siv cov txheej tsim nyog nrog cov tuab txaus kom ua kom txias zoo ib yam.
- • Ua kom pwm ua haujlwm kub yog tias tsim nyog.
- • Siv txoj kev inclined pouring kom zoo dua ntws.
- • Xav txog txhua yam kev co thaum lub sij hawm hlau casting kom txo tau qhov tsis xws luag.
6. Blister (Xuab zeb qhov)
Nta: Cov hlwv yog qhov tsis tu ncua uas pom nyob rau saum npoo los yog sab hauv, zoo li cov xuab zeb nplej. Cov no tuaj yeem pom ntawm qhov chaw, qhov chaw uas koj tuaj yeem tshem tawm cov xuab zeb feem ntau. Ntau cov xuab zeb qhov tuaj yeem muab qhov chaw zoo li txiv kab ntxwv tev zoo li kev ntxhib los mos, qhia txog cov teeb meem hauv qab nrog cov xuab zeb cores lossis pwm npaj.
Ua rau:
- • Xuab zeb core nto tej zaum yuav plam nplej, uas tau encased nyob rau hauv hlau thiab tsim qhov.
- • Lub zog ntawm cov xuab zeb tsis txaus, scorching, lossis kho tsis tiav tuaj yeem ua rau hlwv.
- • Cov xuab zeb tsis sib haum thiab qhov loj ntawm cov pwm txheej tuaj yeem ua rau cov xuab zeb crushing.
- • Pwm dipping hauv cov xuab zeb graphite dej ua rau muaj teeb meem saum npoo.
- • Kev sib txhuam ntawm cov xuab zeb cores thiab ladles lossis cov neeg khiav dej num tuaj yeem ua rau cov xuab zeb paug hauv cov kab nrib pleb.
Txoj kev tiv thaiv:
- • Ua cov xuab zeb cores raws li cov txheej txheem nruj thiab xyuas kom zoo tsis tu ncua.
- • Xyuas kom cov xuab zeb core thiab cov pwm sab nrauv sib phim kom tsis txhob crushing.
- • Ntxuav cov graphite kom sai kom tsis txhob muaj kab mob.
- • Txo kev sib txhuam ntawm cov ladles thiab cov xuab zeb cores kom tsis txhob muaj cov xuab zeb paug.
- • Ntxuav cov kab noj hniav kom huv si ua ntej muab cov xuab zeb cores kom tsis txhob muaj cov xuab zeb xoob xoob.
Yog xav paub ntxiv txog casting qhov tsis xws luag thiab lwm yam kev daws teeb meem, thov hu rau peb ntawm info@dinsenmetal.com. Peb nyob ntawm no los pab koj nrog koj cov kev xav tau casting thiab muab kev taw qhia txog kev txo qis hauv koj cov txheej txheem ntau lawm.